Controlling of Baby Soothers Thickness with Heat Sensitized Latex
John Woon (Senior Latex Consultant): There are so many factors involved in this dipping process that could lead to inconsistent thickness of your products. Briefly, some of these factors are as follows:
1) Latex pH must be closely controlled and monitored before and after the addition of the heat sensitizer.
2) Former temperature should be high enough to ensure good pick of latex but must be well controlled so that a latex dwell time of only a few seconds should suffice.
3) Latex temperature should be at around 20°C and must not vary for more than 1°C.
4) Prevulcanised latex offers better control of product thickness compared to post-vulcanisable latex compounds.